Metal materials · selection guide · for R&D and purchasing
And the same 6061 is 125 MPa annealed and 310 MPa in T6 — the temper code matters as much as changing the alloy.
“Give me an aluminium plate” is a common request in inquiries, and an easy one to get wrong. Aluminium is divided into several series by its main alloying element, with tensile strength anywhere from 90 MPa to 570 MPa; even more often overlooked is the temper code after the grade — the same grade in different tempers can differ by two and a half times in strength. This article puts the strength, properties and uses of common aluminium on one table and explains what temper codes mean.
1. Strength of four common aluminium materials
| Series / grade | Main alloying elements | Tensile strength (MPa) | Properties | Common uses |
|---|---|---|---|---|
| 1xxx pure aluminium (e.g. 1100) | Al ≥99% | 90 (O) to 165 (H18) | Good electrical and thermal conductivity, excellent ductility, good corrosion resistance, lower strength | Foil, conductors, deep-drawn parts, chemical vessel linings |
| 5052 | Al–Mg | 195 (O) to 290 (H38) | Good corrosion resistance (especially marine), good formability, not heat-treatable | Sheet metal parts, enclosures, outdoor and marine parts |
| 6061 | Al–Mg–Si | 125 (O) / 240 (T4) / 310 (T6) | Heat-treatable, good machinability and versatility | Structural parts, fixtures, mechanism parts |
| 7075 | Al–Zn | 230 (O) / 570 (T6) | Highest strength of the four; generally not recommended for welding; more sensitive to stress corrosion | Highly loaded structural parts, mold parts |
Values are typical figures from common specifications; go by the mill certificate. JIAHON’s aluminium covers pure aluminium (99.5–99.95%) and the alloys 5052, 6061 and 7075.
2. Temper codes (O / H / T) matter more than you think
The part after the grade is not a serial number; it determines how hard the material is now:
- O = annealed. Soft, easy to form, lower strength.
- H = strain-hardened. Strength raised by cold working; the higher the following digits, the harder (H32, H34, H38). Used for non-heat-treatable grades such as 5052.
- T = heat-treated. T4 is naturally aged, T6 artificially aged. Used for heat-treatable grades such as 6061 and 7075.
Why this comes first: 6061-O is 125 MPa and 6061-T6 is 310 MPa — a 2.5× difference within one grade. If a drawing says only “6061” without a temper, the finished part may fall far short of the strength you need. Give both grade and temper when inquiring.
Related products: metal sheet series (pure aluminium sheet), metal alloy sheet series (aluminium alloy sheet 5052 / 6061 / 7075), metal rod series (aluminium rod).
3. When to use pure aluminium instead of an alloy
Alloys are stronger, but the added elements lower conductivity, thermal conductivity and corrosion resistance. For these needs, pure aluminium is the right choice:
- Conductors: pure aluminium’s resistivity is about 26.5 nΩ·m. For the same current capacity, an aluminium conductor weighs roughly half as much as copper — which is why aluminium is used for lightweight conductors.
- Deep drawing, bending, foil: pure aluminium has excellent ductility.
- Evaporation, melting, lab feedstock: what matters is purity, not strength.
Related products: metal wire series (aluminium wire), metal pellet series (aluminium / zinc pellets), metal block series (aluminium blocks), metal foil series (aluminium foil).
4. Match your need in the table
| Your need | Material and temper | Product on our site |
|---|---|---|
| General structural parts, fixtures, mechanism parts | 6061-T6 | Aluminium alloy sheet, aluminium rod |
| Sheet metal, enclosures, outdoor or humid environments | 5052 (H32 or harder) | Aluminium alloy sheet |
| High load, high strength | 7075-T6 | Aluminium alloy sheet |
| Electrical and thermal conduction, deep drawing | Pure aluminium | Pure aluminium sheet, aluminium wire |
| Evaporation, melting, lab feedstock | Pure aluminium (pellets / blocks) | Aluminium pellets, aluminium blocks |
| Lightweight shielding, lab support mesh | High-purity aluminium mesh | Metal mesh series (titanium / aluminium mesh) |
| High-porosity carriers, energy absorbers | Aluminium foam | Metal foam series (titanium / iron / aluminium / silver) |
| Mold blasting, matte finishing of fixtures | Aluminium cut wire shot (for blasting) | Aluminium cut wire |
5. FAQ
What is the difference between 6061 and 7075? Do I have to use 7075? The difference is strength versus trade-offs. 6061-T6 is about 310 MPa and 7075-T6 about 570 MPa, but 7075 is generally not recommended for welding, is more sensitive to stress corrosion and costs more. For general structural parts and fixtures, 6061-T6 is enough; switch to 7075 only for highly loaded parts that clearly need the strength.
How do I choose between 5052 and 6061? By forming and environment. 5052 is not heat-treatable and has good formability and corrosion resistance — good for bent sheet metal, enclosures and outdoor parts. 6061 can be heat-treated to T6, is stronger and machines well — good for structural and mechanism parts. Bending: 5052; machining and strength: 6061.
Does aluminium rust? It oxidizes, but the oxide protects it. In air aluminium naturally forms a dense oxide film of about 5 nm that blocks further attack by oxygen, water and dilute acids — passivation. So a “hazy” aluminium surface is usually that protective film rather than worsening corrosion; what to watch are strongly alkaline environments and galvanic corrosion from contact with other metals.
Is aluminium attracted to magnets? No. Aluminium is paramagnetic and barely responds to static magnetic fields; in practice it is treated as non-magnetic. Where measuring equipment or field-sensitive fixtures need non-magnetic materials, aluminium, pure copper and titanium are all options. Further reading: Pure titanium or titanium alloy TC4?, copper, brass, bronze or cupronickel: how to choose.
The drawing only says “aluminium.” What should I add when inquiring? Three things: grade (pure aluminium / 5052 / 6061 / 7075), temper (O / H3x / T4 / T6) and service environment (outdoor, humid, chemical contact). The temper is often left out, yet it can make the same grade differ by two and a half times in strength.