All four are called “copper”, yet their conductivity differs by more than 20 times. First decide whether you need conductivity, machinability, spring properties or corrosion resistance.
JIAHON engineering team · about 8 minutes
When a drawing says “copper”, it may mean four very different materials. Pure copper has a conductivity of 100% IACS; cupronickel can be as low as 4.6%, more than 20 times lower. Choosing the wrong one does not just cost a little more: a whole batch of parts may be unusable.
This guide puts the composition, electrical and thermal conductivity, strength and uses of the four types in one table, and explains when to change material and when you only need to change thickness.
1. Get the names right: “purple copper” = pure copper = red copper
In Chinese, 紫銅 (“purple copper”) means commercially pure copper with at least 99.9% Cu, named after the purplish-red color of its oxidized surface. In Taiwan, shop floors and drawings usually say red copper or pure copper, while specifications from mainland China usually say purple copper. In English it is pure copper or red copper. All three names mean the same class of material.
Note the difference in category: pure copper is a pure metal, while brass, bronze and cupronickel are copper alloys. Adding a second element changes the properties, and each one costs some conductivity.
Composition in one line: pure copper = Cu | brass = copper + zinc | bronze = copper + tin (phosphor bronze adds phosphorus) | cupronickel = copper + nickel
2. The four types compared
| Type | Main composition | Typical grades | Conductivity (% IACS) | Thermal conductivity (W/m·K) | Tensile strength (MPa) |
|---|---|---|---|---|---|
| Pure copper | Cu ≥ 99.9% | C1100 electrolytic tough pitch; C1020 oxygen-free | 100 / 101 | 397 | 220–410 |
| Brass | Cu-Zn | C2600, C2800 | 27–28 | 116–123 | 320–680 |
| Bronze (phosphor bronze) | Cu-Sn-P | C5100, C5210 | 13–15 | 62–84 | 320–970 |
| Cupronickel | Cu-Ni | C7060 (90/10), C7150 (70/30) | 4.6–9 | 29–45 | 290–570 |
Values are reference ranges for common grades in different tempers (soft, half-hard, hard). Always follow the material certificate. Conductivity is given in IACS (International Annealed Copper Standard); 100% IACS is the conductivity of annealed pure copper.
3. Four decisions: choose by what you need
3.1 Electrical or thermal conductivity, or EMI shielding → pure copper
The conductivity of the four types is roughly 100 : 28 : 14 : 6. That is a multiple, not a few percent. If a conductor strip changes from pure copper to brass with the same cross-section, its resistance becomes almost four times higher, and so does the heating.
A common mistake on the shop floor is to change a conductor to brass because pure copper is soft and might not be strong enough. The strength goes up, but conductivity drops to less than a third.
The better solution is usually not a different material but a thicker one. At a fixed width, doubling the thickness doubles the cross-section, halves the resistance and reduces heating. Thicker pure copper makes much more sense than brass. The actual current capacity must be calculated from the allowed temperature rise and cooling conditions.
3.2 Heavy turning or forming → brass
Pure copper is “sticky” to cut: it easily forms built-up edge and shortens tool life, so it is not suited to high-volume turning and milling. Adding zinc greatly improves machinability, which is why terminals, sleeves, valves and hardware parts are mostly brass.
The cost is conductivity of 27–28% IACS and thermal conductivity around 120 W/m·K. If a part must both conduct and be machined, the usual solution is a brass body with a plated contact surface, or a brass body with a crimped pure copper terminal, rather than turning the whole part from pure copper.
3.3 Springs and repeated loading → bronze (phosphor bronze)
Spring contacts and connector contacts need more than “springs back when pressed”: they must still spring back after six months of use. That is resistance to stress relaxation.
Annealed pure copper has almost no spring. Brass has some but relaxes over time. Phosphor bronze (Cu-Sn-P) can reach tensile strengths above 900 MPa and resists stress relaxation clearly better than brass, so it is the standard choice for spring contacts. Its good wear resistance also makes it common for bushings and sliding parts.
Its cost is conductivity of 13–15% IACS. Contacts that must both conduct and spring usually rely on plating on the contact surface, not on the base metal.
3.4 Corrosion resistance, especially seawater and heat exchange → cupronickel
Cupronickel is a copper-nickel alloy, commonly 90/10 (C7060) and 70/30 (C7150). In seawater it forms a stable protective film and resists erosion and biofouling well, so ship piping and seawater heat exchanger tubes are its main uses.
With conductivity of 4.6–9% IACS and thermal conductivity of 29–45 W/m·K, it is the lowest of the four. On the other hand, its high resistance and low temperature coefficient of resistance make copper-nickel alloys common as resistance materials and in thermocouples.
4. Two points that are often missed
4.1 When oxygen-free copper is necessary, and when it just costs more
A common belief is that oxygen-free copper conducts better and is therefore “higher grade”. The real numbers: electrolytic tough pitch copper (ETP, C1100) is 100% IACS; oxygen-free copper (OFC, C1020 / C10200) is 101% IACS. A 1% difference does not matter for most applications.
The real reason to specify oxygen-free copper is hydrogen embrittlement. ETP copper contains about 0.02–0.04% oxygen, present as cuprous oxide. When it is heated above about 370 °C in a hydrogen-containing reducing atmosphere (hydrogen furnace annealing, some brazing processes, vacuum or reducing furnaces), hydrogen reacts with the cuprous oxide to form water vapor, which creates voids at grain boundaries and makes the material brittle and crack. Oxygen-free copper keeps oxygen below 10 ppm, so this reaction does not occur.
- General conduction, grounding, shielding at room temperature → C1100 ETP copper is enough.
- Hydrogen furnace, brazing, vacuum or reducing atmosphere above about 370 °C → specify oxygen-free copper C1020 / C10200.
4.2 Magnetism: none of the four is ferromagnetic
For measuring equipment, medical devices and magnetically sensitive fixtures, this can matter more than conductivity. Pure copper, brass and bronze are non-ferromagnetic. Cupronickel contains nickel, but the common 90/10 and 70/30 compositions are also not ferromagnetic; iron in the formula can raise permeability slightly. If your application has a permeability limit, please include it in your inquiry.
5. Match your need to a material
| Your need | Recommended material |
|---|---|
| Conductor strips, ground plates, busbars | Pure copper |
| EMI shielding | Pure copper |
| Heat spreading | Pure copper |
| EDM electrodes, plating racks, ground rods | Pure copper |
| Copper plating, electroforming feedstock | Electrolytic copper |
| Research electrodes, current collectors | Pure copper / oxygen-free copper |
| High-volume turned parts, terminals, sleeves | Brass |
| Spring contacts, connector contacts | Bronze (phosphor bronze) |
| Seawater piping, heat exchanger tubes | Cupronickel |
| Hydrogen furnace, brazing, vacuum or reducing atmosphere | Oxygen-free copper |
6. FAQ
Are “purple copper” and red copper the same material? Yes. Both mean commercially pure copper with at least 99.9% Cu; only the names differ. Taiwan usually says red copper or pure copper, drawings and specifications from mainland China say purple copper, and English uses pure copper or red copper.
Can brass replace pure copper for a conductor strip? Not for conduction. Brass is about 27–28% IACS, a little over a quarter of pure copper, so with the same cross-section the resistance is almost four times higher and heating rises. If the reason for changing is strength, keep pure copper and make it thicker, which increases the cross-section and reduces resistance and heating. Current capacity must still be calculated from the allowed temperature rise and cooling.
Is oxygen-free copper always better than ETP copper? No. The conductivity difference is only 1% (101% vs 100% IACS), so ordinary room-temperature conduction, grounding and shielding do not need oxygen-free copper. You need it for processes that heat the copper above about 370 °C in a hydrogen-containing reducing atmosphere, such as hydrogen furnace annealing, some brazing, or vacuum or reducing furnaces, because ETP copper suffers hydrogen embrittlement under these conditions.
The copper surface has tarnished. Can it still be used? In most cases, yes. Bare copper turns from orange-red to dark brown in air. This oxide film has little effect on the conductivity of the conductor itself, but it raises contact resistance at contact surfaces. If your application controls contact resistance, crimp or solder soon after fitting and do not leave it exposed for long. If the part will be soldered or ground later, ordinary storage tarnish does not affect use.
The drawing only says “copper”. How do I tell which one? Start with the use: conduction, heat and shielding are almost always pure copper; turned parts, terminals and valves are mostly brass; springs and contacts are phosphor bronze; seawater and heat exchanger piping is cupronickel. Then look for a grade: C1xxx is pure copper, C2xxx brass, C5xxx bronze and C7xxx cupronickel. If neither is given, describe the use in one sentence when you ask for a quote; it is more reliable than guessing a grade.
Copper selection and specification check
If you have a drawing but are not sure the grade is over-specified, or want to check whether thickness and current capacity are enough, send us the use, working temperature, later processes and quantity, and we can help you evaluate. Contact JIAHON →