When boards come out of wave soldering with defects, look at the appearance first, then decide where to check: round balls are solder balls, spikes are icicles, adjacent joints joined together are bridging, holes in the joint are blow holes (pin holes), and solder that has not climbed all the way up the through-hole is poor hole fill. The first suspect differs for each of the five: for solder balls and pin holes, mostly check preheat, moisture and flux first; for icicles and bridging, check the flux, the state of the solder pot and the peel-off conditions first; for poor hole fill, check preheat, flux penetration into the hole and the board’s surface finish first. This article follows the three stations of solder paste printing, nozzles and feeders, and adds the wave soldering station for through-hole components; use the two tables to match symptoms first, then dig further.
Figure 1: The wave soldering line process and the stations where each defect commonly arises (schematic). Process, in the conveying direction: flux application (spray or foam) → preheat (heating) → contact with the solder wave (nozzle plate, impeller shaft) → peel-off (the moment the solder is pulled away) → cooling (the solder solidifies). Defects commonly caused at each station: flux application — poor hole fill (flux did not penetrate the hole, insufficient preheat); preheat — solder balls (solvent not driven off); wave contact — poor hole fill (did not properly touch the wave, contact time too short), bridging; peel-off — icicles, bridging, solder balls (spatter as the solder falls back into the pot); cooling — blow holes / pin holes (gas escaping as the solder solidifies). Conditions brought in before the board enters the line: moisture in the board, through-hole copper plating, solder mask cure, number of heat exposures of the OSP (reflow history) — linked to blow holes / pin holes, solder balls and poor hole fill. Schematic; each defect can also be caused at other stations; no temperature, speed or angle values are shown.
1. First identify which type it is: board symptom lookup
Table 1 | Board symptom → what to check first
| What you see on the board | Name | Check first | Other common causes |
|---|---|---|---|
| Separate small round balls of solder on the board surface | Solder balls; IPC-A-610 §5.2.7.1 | Whether preheat is sufficient, whether the flux solvent was driven off before contact with the wave; whether too much flux was applied | Solder mask too thin, under-cured or incompatible with the flux; moisture in the board, high humidity in the workshop; large drop or unstable wave at the peel-off end |
| Spikes pulled out at the tip of the joint | Icicles, solder projections; IPC-A-610 §5.2.10 (revisions F, G), §5.2.11 (revision H) | Amount and evenness of flux; whether the measured solder pot temperature is low | Dross sticking to the leads, contaminated solder; leads too long, unsuitable hole-to-lead ratio; board or components drawing too much heat (large ground planes) |
| Adjacent joints joined into one by solder | Bridging, solder shorts; IPC-A-610 §5.2.7.2 | Amount and evenness of flux; preheat; conveyor angle, contact time and wave separation | Leads too long or bent, small pad spacing; dross and contamination; worn or blocked nozzle plate |
| Small holes or bubbles on the surface or inside the joint | Blow holes, pin holes; IPC-A-610 §5.2.2 | Whether the board contains moisture (absorbed moisture, stored too long); thickness of through-hole copper plating, and voids | Insufficient preheat, flux solvent not dry; foreign matter in the hole, solder mask in the hole |
| Solder has not filled the through-hole; no fillet visible on the component side | Poor hole fill, insufficient topside fillet; IPC-A-610 §7.3.5.1 Vertical Fill | Preheat; whether the flux penetrated into the hole; whether the board properly touched the wave (wave height, fingers and carrier) | Contact time too short (conveyor speed, conveyor angle); solder pot temperature low or contaminated; OSP board with many heat exposures, through-hole copper plating, hole-to-lead clearance |
The order of “Check first” is a common troubleshooting habit (check the items that are easy to confirm first), not a requirement of a standard. IPC-A-610 section numbers differ slightly between revisions; the acceptance criteria follow the revision you use, the Class level and the customer specification.
2. Before you start, narrow the scope
Look at the location: if the whole batch and the whole board show the same defect, first suspect the board and upstream conditions (preheat, flux, moisture in the board); if it concentrates on a few specific components, first look at lead length, hole diameter and pad design. This is engineering judgment, not a requirement of a standard.
Confirm it was caused by wave soldering: reflow also produces solder balls. If the board has gone through both reflow and wave soldering and the solder balls fall mostly around SMD components, usually go back and check the printing station first; for the order, see “How to Troubleshoot Solder Paste Printing Defects?“.
Measure the actual temperature first: the preheat set point does not necessarily equal the actual board surface temperature; measure with a profiler before drawing conclusions.
3. Check items for process and material condition
Table 2 | Check item → symptoms commonly linked when it deviates
| Check item | What to confirm | Symptoms commonly linked when it deviates |
|---|---|---|
| Preheat | Measure the board surface temperature profile with a profiler (for the measurement method, see IPC-7530), not just the machine set point; the reasonable range varies with the flux type and the board’s thermal mass, and follows the flux TDS (technical data sheet) | Solder balls, bridging, pin holes, poor hole fill |
| Flux | Whether the flux unit works normally, whether the spray is even and reaches into the holes; whether the amount applied and the specific gravity have drifted | Solder balls, icicles, bridging, poor hole fill |
| Solder pot temperature and solder condition | Measure the solder pot temperature; skim off dross; when the solder is contaminated with impurities, replace or top up the solder | Icicles, bridging, poor hole fill |
| Wave and peel-off conditions | Whether the wave is flat and stable; wave height, contact time, conveyor angle; whether the nozzle plate is worn or blocked | Solder balls, icicles, bridging, poor hole fill |
| Board | Moisture (storage, workshop humidity); through-hole copper plating thickness and voids; solder mask cure; number of OSP heat exposures | Solder balls, pin holes, poor hole fill |
| Components and design | Lead protrusion length, hole-to-lead clearance, pad spacing, component solderability | Icicles, bridging, poor hole fill |
| Carrier and fingers | Carrier overheated, damaged or poorly designed; fingers worn or damaged | Poor hole fill |
This article does not list temperature or speed figures: the ranges given in different technical documents vary with the flux type, the alloy and the board, and applying them directly can easily lead to misjudgment. For values, please follow the flux TDS, the solder material data and your own process validation.
4. Notes on the five defects
Solder balls and pin holes: look at solvent and moisture first
One of the tasks of preheat is to drive off the flux solvent before the board touches the wave; otherwise the solvent spatters the moment it contacts the wave, forming solder balls. Solder mask that is too thin, under-cured or incompatible with the flux is also named as a cause.
Pin holes, on the other hand, are gas escaping as the solder solidifies. The gas mostly comes from moisture in the board; if the through-hole copper plating is too thin or has voids, the moisture has a way out. So pin holes are often related to incoming material and storage, and adjusting the solder pot alone may not solve them. Baking the boards can drive off moisture, but it treats the symptom, and some technical documents warn that baking may affect solderability. Whether to bake and how, please confirm with the board maker first.
Icicles and bridging: look at the moment of peel-off — does the solder drain cleanly?
The causes of the two overlap heavily: insufficient or uneven flux, low solder pot temperature, dross sticking to the leads, and leads too long. Bridging has an extra design aspect: large pads and long leads hold solder, and if the conveyor angle, contact time or wave separation is not smooth, the solder does not drain and joints are bridged. A common practice on the design side is to add a solder thief pad at the trailing end.
The shape of the wave and the distribution of solder are determined by the nozzle plate; once the nozzle holes are worn or blocked, the incidence of defects such as solder bridges rises noticeably (see section 5).
Poor hole fill: first see whether it can get in; OSP boards have one more check
For the solder to fill the through-hole, preheat has to be adequate, the flux has to penetrate the hole first, the board has to properly touch the wave, and the contact time has to be long enough. One technical document points out that it is common for hole fill to get worse after switching the flux from foam to spray, because spray penetrates into the holes less well; confirm that the inside of the holes is reached.
OSP boards have one more check: the OSP protective film degrades with heat, and if the board has gone through reflow first (especially double-sided boards) before wave soldering, it is harder for solder to wet the inside of the holes; one study lists the number of reflow passes as a significant factor in hole fill. You can start by controlling the time between reflow and wave soldering, confirming that the flux activity is sufficient, and asking the board maker to confirm the OSP film thickness specification.
For acceptance, IPC-A-610 sets requirements for vertical fill of through-holes (§7.3.5.1 Vertical Fill) by Class level and revision; please follow the revision you use and the customer specification.
5. Consumable parts that affect defects: nozzle plates, titanium fingers, solder bars
At the end of troubleshooting, there are a few parts that have to be replaced once worn.
The nozzle plate determines the shape of the wave and the distribution of solder; once the nozzle holes are worn or blocked, the incidence of defects such as solder bridges rises noticeably. Jiahon has compatible wave soldering nozzle plates covering several brands of machines; please give the machine model and size, or send the actual part for confirmation.
Titanium fingers hold the board as it passes over the solder pot; they withstand high temperature and resist solder erosion, and are high-consumption spare parts; one technical document also lists damaged fingers as a check item for poor hole fill. There is also the impeller shaft bearing housing, whose wear leads to an unstable wave. See compatible wave soldering titanium fingers and titanium fingers and bearing housings.
Solder bars: once impurities and dross in the solder build up to a certain level, top up or replace the solder. Jiahon stocks solder bars for wave soldering; the specification column of the product page lists several types, 1 kg per unit; for the differences between types and prices, please inquire.
The specification of each of these parts has to be confirmed by machine model. Give us the machine model, size or a photo of the actual part, and Jiahon can help match it; for more wave soldering and reflow consumables, see Reflow oven and wave soldering consumables and spares.
Further reading
To go through the related process steps together, you can read these next:
Related products mentioned in this article
Specifications are as on each product page; for actual configuration, prices and lead times, please inquire.
SMT reflow profiler Q12 / Q24: multi-channel K-type thermocouples record oven temperatures simultaneously; the “applicable processes” column on the product page lists SMT reflow, wave soldering and selective wave soldering; requires a thermal barrier box (sold separately). View product
Standards referenced
For the standards cited in this article, please follow the current revision from each publishing body.
IPC-A-610F “Acceptability of Electronic Assemblies” (table of contents)
Publisher: IPC (Global Electronics Association)IPC-A-610G “Acceptability of Electronic Assemblies” (table of contents)
Publisher: IPC (Global Electronics Association)IPC-A-610H “Acceptability of Electronic Assemblies” (table of contents)
Publisher: IPC (Global Electronics Association)IPC-7530B “Guidelines for Temperature Profiling for Mass Soldering Processes (Reflow and Wave)” (table of contents)
Publisher: IPC (Global Electronics Association)
This article is a summary of the general case; the actual causes and settings still depend on the individual case. Please follow the technical documents of your flux, solder and equipment suppliers, and your own process validation.