How to Choose Solder Paste: With a Few Candidates in Hand, 5 Verification Stages from Data Sheet to Pilot Run

The order for choosing solder paste: first use the data sheet to drop obvious misfits, then compare how stable the printed volume is, then reflow, check residue and reliability, then run a small pilot. At every stage, use the paste you use now as the control.

  • Compare printing first: one paper cites an industry view that over 60% of end-of-line defects trace back to paste and printing, with about another 15% added by reflow. So the first comparison is printed paste volume.
  • Rank in two tiers: items that directly affect yield and output come first, and failing one eliminates the candidate; items that only affect handling convenience, such as storage temperature and warm-up time, decide between two close candidates.
  • Have a control: test every candidate under the same conditions as your current paste; numbers from one paste alone have nothing to compare against.

For paste composition and how to read the label, see How to read solder paste composition and specs; for mixing and life after opening, see How long to stir solder paste, and how to set its life after opening. This article starts from “two or three candidate pastes in hand, one to choose”: what to compare first, how, and how far before switching. Each stage covers what to do and how JIAHON can help; sources and limitations are in the notes at the end.

Stage 1: A first cut on the data sheet

Data sheet figures are measured by the supplier; their purpose is to decide who is worth trying on the line, not who wins. One paper’s view is that most paste makers do standard tests conscientiously, so data sheets can be used for screening, but for the last few candidates it is preferable to verify some items yourself.

What to checkHow to handle it
Alloy, powder size (Type 3, Type 4), metal contentCandidates should match your current process; if not, it is not a like-for-like comparison
Flux type and halogenNo-clean or water-soluble, halogen-containing or not: match your process and customer requirements first
J-STD-004, J-STD-005 test resultsCopper mirror corrosion, halides, SIR (surface insulation resistance), slump, solder balls, tack, wetting: tested or not, passed or not, third-party report or not
Usage conditionsStorage temperature, warm-up time, stencil life, plant temperature and humidity requirements, reflow profile requirements

Ranking: two tiers. This is a working approach, not a standard; adjust your ranking to your product and line.

  • Tier 1, failing one eliminates: viscosity, stencil life, whether it spatters under rapid heating, whether solder climbs high enough on the joint, how long post-reflow residue can wait before cleaning (water-soluble types only).
  • Tier 2, deciding between close candidates: storage temperature, warm-up time, number of reflow profile requirements, plant environment requirements, whether offset parts self-align in reflow, wash water temperature.
  • Stencil life, warm-up time and the number of profile requirements can differ considerably between pastes, so these data sheet columns are worth looking at first.

How JIAHON can help: the solder paste / solder wire series page lists SAC305 and Type 4 pastes and various solder wires; ask about other alloys, powder sizes, flux types, packaging and data sheets.

Stage 2: Printing — compare “is the printed volume stable?”

Printing is where pastes differ most, and it affects yield downstream. One paper’s approach screens on this alone first: if volume is unstable or print shape poor, drop the candidate without further testing.

What to testHowWhat to look at
Volume and stabilitySame stencil, same print settings, print 10 boards in a row (4 if short of time) without wiping, measure paste volume at each apertureHigh mean volume, small standard deviation
Pause and printAfter printing, pause 1 hour without mixing, print another round; repeat (cumulative 2, 4, 8 hours)How much volume drops, how much bridging
Print speedPrint one round at normal speed and one at an occasional faster speed, e.g. 25 mm/s and 50 mm/sHow much volume drops and standard deviation changes at higher speed
Small aperturesTake apertures with area ratio (aperture area / aperture wall area) 0.3–0.8 and look for insufficient solderFew apertures short of solder
Left out after openingSpread 30–50 g thinly in a container beside the printer, weigh at 8 and 24 hoursSmall weight change; gain usually means moisture uptake, loss usually solvent evaporation

Without SPI (solder paste inspection), one paper’s alternative uses an electronic balance: weigh each board before and after printing, calculate grams printed per board, and compare mean and standard deviation. It cannot show which aperture has the problem, but is enough to compare total volume between pastes.

How JIAHON can help:

Stage 3: Reflow — how well it solders, how wide the window

Reflow with real boards and parts, not only test boards. First run each candidate and the current paste once on your standard profile; for those remaining, change the profile and see whether they still hold up.

What to look atHowWhat good looks like
Wetting and solder ballsMicroscope on pads and beside partsFull pad wetting, few small solder balls beside parts
VoidsX-ray under QFN and BGAFew, small voids
Head-in-pillowAfter BGA reflow, check whether ball and paste fused into oneNone
Solder climb and tombstoningCheck joint climb height and whether small parts stand upEnough climb, no tombstones
Spatter under rapid heatingRaise the ramp rate and reflow againNo spatter; under the same heater settings, the quicker the conveyor can run, the more boards per hour
Profile windowLow, medium and high profiles, each also with nitrogen on nitrogen linesGood soldering on every one

The wider the profile window, the better. One paper combined three peak temperatures with three times above liquidus into nine profiles and required one paste to solder well on all nine; in the research it cites, only one paste passed all nine. More profile requirements also make a paste harder to manage, and under the same heater settings a paste that spatters forces a slower conveyor.

How JIAHON can help:

Stage 4: Residue and reliability — what stays after reflow

Decide the route first: residue stays on the board (no-clean), or is washed off after reflow (water-soluble). The two need different additional tests.

RouteCharacteristics compared in papersAdditional tests
No-clean, residue staysMore robust than water-soluble, wider print window; if conformal coating or underfill goes over the residue, test the combinationSIR; compatibility tests of coating, underfill and residue
Water-soluble, washed offUsually good wetting, but sensitive to temperature and humidity, shorter stencil life, narrower print window; solder balling worsens if boards wait long between print and reflowIonic residue after washing, to confirm cleaning
  • Water-soluble vs. no-clean: one paper compared 6 pastes (3 water-soluble, 3 no-clean); water-soluble types performed worse overall and needed more careful storage and handling; the paper notes its sample was limited.
  • Conformal coating: another paper concludes that conformal coating can go over no-clean residue on most assemblies, but compatibility tests are essential to confirm the coating really protects and meets the product’s use conditions.
  • Underfill: another paper paired different no-clean residues with underfills and tested SIR; results varied by combination, and one underfill had clearly worse SIR. So materials must be verified as a set, not from single-material data.
  • Clean or not: for identifying white residue and deciding whether to clean, see Does flux residue need cleaning?

How JIAHON can help:

  • JHPB-TLZ20 ionic contamination tester: extracts with 3:1 isopropanol / deionized water at 40±1°C, measures conductivity and ion concentration, outputs a report automatically; boards up to 350 × 600 mm.
  • Constant temperature and humidity chamber: JHHWS-260BE, 0–70°C, 30–98% RH, 260 L, 24-segment programmable. If your test conditions exceed this range, ask about high-temperature, high-humidity versions.

Stage 5: Pilot run and introduction

After the first four stages, one or two candidates usually remain. The final stage runs on the real line:

  • Pilot run: pick one line and one product; run several consecutive lots each of the candidate and the current paste, on both day and night shifts. Record defect type and count per lot: tombstones, component offset, missing parts, opens, bridging, others separately; convert to ppm to compare. Photograph each step (after printing, after placement, after reflow, and after washing for water-soluble types) so there is a basis to look back on.
  • Turn the results into one decision: use a scoring sheet. Give each item a weight (3 = critical, 2 = secondary, 1 = minor) and each candidate a score per item (3 = better, 1 = worse), multiply and add. The figures below show the method only, not test results.
ItemWeightCandidate A scoreCandidate B scoreA totalB total
Print volume stability33296
Reflow joints32369
Pause and print23162
Warm-up time11313
Total2220
  • When customer specs apply: changing paste is often treated as a change requiring customer notification. Customers typically look at three things: samples made with the new paste, reliability tests (high temperature/humidity and temperature cycling), and an audit of the paste supplier.
  • Paste maker changes formula or production site: the flux standard (J-STD-004C) has requalification clauses for formula and site changes; see the standard for details. In practice, ask the supplier to include such changes in written notifications.
  • On the floor after introduction: for storage, first-in-first-out, warm-up and mixing, see How long to stir solder paste, and how to set its life after opening.

How JIAHON can help:

For solder paste, solder wire, SPI evaluation, electronic balances, ionic contamination testers, humidity chambers or paste management equipment, contact JIAHON or email [email protected].

Notes: sources and limitations

  • Papers: the approaches above come from published papers on paste evaluation (print-first screening and the cited 60%/15% figures; scoring sheet and control comparison; screening plus robustness with three profiles in air and nitrogen; supplier sample conditions under J-STD-004/005; the nine-profile window; water-soluble vs. no-clean; conformal coating; underfill SIR pairing). Their alloys, equipment and dates differ, so results cannot be applied directly to your product; use them for the order and method of comparison.
  • Standards: for pass/fail values, see the official texts; this article does not restate them. J-STD-004C covers copper mirror, corrosion, halide content and SIR (3.3.1.1–3.3.1.4) and requalification on formula or site change (4.3.3–4.3.3.2); J-STD-005B covers powder size, metal content and viscosity (3.4–3.6) and slump, solder balls, tack and wetting (3.7–3.10). See the IPC J-STD-004C table of contents; go by each issuing body’s current edition.
  • Data sheet figures: mostly typical values; some data sheets state they are for reference only and not for incoming specifications. Set incoming specs separately with the supplier.
  • Equipment: JIAHON has no X-ray or cross-section lab equipment; these must be outsourced.
  • Scoring sheet figures: illustration only.