Solder paste is a mixture of alloy powder and flux: metal powder makes up about 85 to 90% by weight (data sheets often say around 88.5%), but because metal is much heavier than flux, it occupies only about half the volume. On a jar’s label and data sheet there are six fields to read: alloy, powder type, metal content, flux type, viscosity and storage conditions — a typical product name reads like “SAC305 T4 88.5%.” This is a general overview; each case needs its own assessment, and actual values for each paste follow the maker’s technical data sheet (TDS).
Table 1: What each component does, and what you typically see when it’s wrong
| Component | Role in the paste | Typical symptoms when wrong or off (general) |
|---|---|---|
| Alloy powder (metal, about 85–90% by weight) | Melts in reflow to form the solder joint. Different alloys melt at different temperatures: leaded Sn63Pb37 about 183 °C, SAC305 about 217–220 °C, bismuth-containing low-temperature alloys about 138 °C | The reflow profile must follow the alloy’s melting point; switching alloys but keeping the old profile may leave the peak below the new alloy’s melting point |
| Resin (rosin) | Main solid in the flux, rosin or synthetic resin; becomes most of the residue after reflow | Affects residue amount and appearance; whether residue must be cleaned depends on product class and acceptance requirements (IPC-A-610) |
| Activators | Remove oxide from pads and leads so molten solder can wet | Too little activity leaves oxide and poor wetting; activator not consumed in reflow may remain and affect electrical reliability |
| Solvents | Dissolve other components and adjust consistency; evaporate during preheat | Incomplete evaporation or too fast a ramp makes volatiles burst out (spattering); the preheat stage must allow for solvent boiling points |
| Rheology additives (thixotropes) | Make paste thin under the squeegee’s shear and thick after printing, so deposits hold their shape | Poor thixotropy or off-spec viscosity: too thick gives insufficient solder, too thin gives slump and bridging |
Table 2: The six label and data sheet fields
| Field | Typical wording (examples from public data sheets and product names; each paste differs) | How to read it | Main process step affected |
|---|---|---|---|
| Alloy | SAC305, Sn96.5Ag3.0Cu0.5 | SAC = tin, silver, copper; 305 = 3.0% silver, 0.5% copper, the rest tin; melts at about 217–220 °C | Reflow profile |
| Powder type | Type 4 / T4 | Higher number = finer powder: Type 3 about 25–45 μm, Type 4 about 20–38 μm, Type 5 about 15–25 μm | Stencil apertures, print release, oxidation |
| Metal content | 88.5 wt% (some give flux content instead, e.g. 11.0 ± 0.5 wt%) | Metal as a weight percentage of the whole; the two figures add to 100% | Solder volume after reflow |
| Flux type | ROL0, ROL1 | RO = rosin-based; L = low activity; last digit 0/1 = halide (0 below about 0.05%) | Residue, cleaning, reliability |
| Viscosity | 160–230 Pa·s (25 ± 3 °C, 10 rpm, spiral viscometer) | Read together with viscometer type, speed, temperature and unit | Aperture filling, release, slump |
| Storage conditions | 2–10 °C, 180-day shelf life, warm up about 3–4 hours before opening | Each paste differs; follow its TDS | Warm-up, first-in first-out, spattering and voids |
1. What’s in solder paste: about nine-tenths metal by weight, one-tenth flux
Solder paste has two parts. The first is alloy powder, which melts in reflow to form the joint. The second is flux (also called the vehicle or carrier), which removes oxide and binds the powder into a paste that prints and holds its shape.
By weight, public sources mostly give 85–90% metal powder, and data sheets commonly around 88.5%. By volume, though, it is roughly half and half: metal is much heavier than flux, so it is nine-tenths of the weight but only half the volume. That is why the solder joint after reflow is only about half the volume of the printed paste.
The flux itself has four kinds of components (Table 1): resin, activators, solvents and rheology additives. Their proportions are proprietary, and public papers and patents give very different ranges — for activators, one paper’s example is about 5% while a patent’s preferred range is 5–30%. So labels and data sheets almost never list component proportions; what you can read are the overall “flux type” and “metal content.”
2. Alloy: breaking down “SAC305”
SAC stands for tin (Sn), silver (Ag) and copper (Cu). SAC305 corresponds to Sn96.5Ag3.0Cu0.5 — 3.0% silver, 0.5% copper, the rest tin.
The alloy determines the melting point: leaded Sn63Pb37 about 183 °C, SAC305 about 217–220 °C, bismuth-containing low-temperature alloys about 138 °C. One data sheet states plainly that the recommended profile depends on the alloy’s melting point and the components’ thermal behavior. So the alloy on the label is the first field to check against your reflow profile.
This article only explains the fields; it doesn’t recommend an alloy — that depends on the product, components and customer specifications.
3. Powder type: the higher the number, the finer the powder
Type is a powder particle size grade, tabulated in IPC J-STD-005. Three common grades (μm): Type 3 about 25–45, Type 4 about 20–38, Type 5 about 15–25 (some sources give 10 as the Type 5 lower limit). Labels often abbreviate them as T3, T4, T5.
Finer powder passes through smaller apertures, at the cost of more total surface area for the same weight. Public data show Type 4 has about 20% more total surface area than Type 3, and Type 5 about 75% more. More surface area means faster oxidation and stricter shelf-life and environmental control.
A commonly quoted rule of thumb is the “five-ball rule”: the minimum aperture width should fit five of the largest particles side by side. Type 4’s upper particle size is about 38 μm, so five come to about 190 μm, or 0.19 mm. This is a rule of thumb, not a standard; verify against your own stencil apertures and process. For apertures and area ratio, see How to troubleshoot solder paste printing defects.
4. Metal content: the 88.5 at the end of the name is a weight percentage
Product names often list alloy, type and metal content in order, such as “SAC305 T4 88.5”; the last number is metal as a weight percentage of the paste.
Some data sheets give flux content instead (for example 11.0 ± 0.5 wt%); the two add to 100%, so you can convert.
For the same alloy, metal content often differs slightly by type. In one public paper’s SAC305 examples, Type 3 was 88.5%, Type 4 88.3%, Type 5 88.0% and Type 6 87.5% — finer powder, lower metal content. The paper also noted that finer-powder formulations had higher flux proportions and some failed hot slump tests. This is a single study, for reference only; each case needs its own assessment.
In practice, for the same printed volume, lower metal content leaves less solder after reflow.
5. Flux type: reading ROL0 and ROL1
IPC J-STD-004 classifies flux with four characters. Taking ROL0:
- RO: base material. RO = rosin, RE = synthetic resin, OR = organic, IN = inorganic, determined by the largest share of non-volatile content by weight.
- L: activity. L low, M medium, H high.
- 0: halide. 0 means below about 0.05%, considered halide-free; 1 means above it. For exact boundaries, follow the current standard.
Three things are easy to misread in this field:
- The classification code doesn’t say whether to clean. ROL0 and ROL1 are often used as no-clean, but whether residue must be cleaned depends on product class and acceptance requirements (IPC-A-610).
- Check which edition was used. If the data sheet doesn’t say J-STD-004A or B, ask the maker; one source notes that a flux marked 0 under the older edition may contain more halide than one marked 1 under the newer edition.
- “Halogen-free” and the 0/1 digit are different measurements. The former refers to halogens, the latter to halides; a halogen-free flux is always halide-free, but not the other way round. This comes from a single source; each case needs its own assessment.
If flux residue must be cleaned after reflow, first confirm whether your flux is rosin, no-clean or water-soluble. JIAHON’s stencil and flux cleaners (JH series) are described for no-clean and rosin flux residues; please tell us your flux type before ordering. For how to clean stencils and to what level, see the SMT stencil cleaning guide (IPC-7526).
6. Viscosity: read the number together with its conditions
Viscosity affects whether paste fills apertures and whether it slumps after printing. Too thick and joints tend to lack solder; too thin and deposits slump and bridge.
Always read data sheet viscosity together with viscometer type, speed, temperature and unit. Two public data sheets as examples: one gives 160–230 Pa·s (25 ± 3 °C, 10 rpm, spiral viscometer), the other 210–300 × 10³ mPa·s (also 10 rpm, 25 °C). They look very different, but 1 Pa·s equals 1,000 mPa·s, so the second is 210–300 Pa·s — the same order of magnitude in a different unit.
Measured viscosity of the same jar also shifts with temperature and stirring: insufficient warm-up or settling makes it deviate from the data sheet. On both, see Tips for warming up syringe solder paste and Solder paste properties, stencil cleaning and logistics control.
7. Storage conditions: every paste is different — follow the TDS
Most solder pastes fall within 0–10 °C refrigeration, but the limits, shelf life and warm-up time before opening differ for each. Two public data sheets as examples: one gives 2–10 °C, a 180-day shelf life and about 3–4 hours’ warm-up; the other 3–8 °C, up to 12 months refrigerated and 4–8 hours’ warm-up. Don’t apply one temperature and time to every product.
Two management steps tie directly to this field. One is warm-up: set JIAHON’s smart solder paste warmer to the warm-up time in that paste’s TDS. The other is shelf life: manage by the data sheet’s limit, with a solder paste first-in first-out fixture so the earliest paste is used first.
8. JIAHON’s solder paste: reading the name, and which fields to ask about
The paste in JIAHON’s solder paste / solder wire series is named “solder paste SAC305-T4,” with a 1 kg unit and a halogen-free marking on the product page. Read field by field:
- SAC305: alloy, 3.0% silver, 0.5% copper.
- T4: by common convention, Type 4 powder.
- Halogen-free marking: as shown on the product page; please ask for the data sheet to confirm.
Metal content, flux type, viscosity, storage conditions, and packaging (jar or syringe) are not stated on the site; please ask.
Related products (specifications follow each product page; please ask about configuration, availability and lead time):
- Solder paste / solder wire series: SAC305-T4 solder paste, 1 kg, plus several lead-free solder wires.
- Smart solder paste warmer: set warm-up time per the paste’s TDS.
- Solder paste first-in first-out fixture: manage by shelf life.
- Stencil and flux cleaners: JH series.
- Solder paste warmer series: for 500 g jars, in 1-, 2-, 4- and 8-position and ten-slot versions; set warm-up time per the paste’s TDS.
- SMT reflow profiler (12 / 24 channels): records temperatures at multiple points in the reflow oven with thermocouples, for new process setup, equipment verification and post-changeover audits; thermal barrier sold separately.
To check the specifications of the paste you have, or for details of the paste on our site, please contact JIAHON or email [email protected].
Standards cited (please use each publisher’s current version):
- IPC J-STD-004C, Requirements for Soldering Fluxes — IPC (Global Electronics Association)
- IPC J-STD-005B, Requirements for Solder Pastes — IPC (Global Electronics Association)
- IPC-A-610, Acceptability of Electronic Assemblies — IPC (Global Electronics Association)